AWS E2209-16 Inkingi zo gusudira mu byuma bitagira umugese, Inkingi zo gusogongera amashanyarazi zipfundikiye mu byuma bitagira umugese

Ibisobanuro bigufi:

AF2209-16 (AWS E2209-16) ni electrode y'icyuma kitagira umugese ifite azote nkeya cyane ifite calcium nyinshi kandi itwikiriwe na titanium-calcium.


Ibisobanuro birambuye ku gicuruzwa

Ibirango by'ibicuruzwa

Gusudira mu byuma bitagira umwandaElectrode

AF2209-16                               

GB/T E2209-16

AWS A5.4 E2209-16

Ibisobanuro: AF2209-16 ni electrode y'icyuma kitagira umugese ifite azote nkeya cyane ifite titanium-calcium coating. Ishobora gukoreshwa haba kuri AC na DC ifite imikorere myiza. Kubera ko irimo molybdenum na azote, kandi ingano ya karuboni ikaba nke cyane, icyuma cyashyizwemo gifite ubushobozi bwo kurwanya ingese no kurwanya ingese, cyane cyane kurwanya ingese.

Ikoreshwa: Ikoreshwa cyane cyane mu gusudira ubwoko bumwe bw'ibikoresho by'icyuma kitagira umukungugu bifite karubone nkeya cyane mu nganda za peteroli n'iz'amazi. Nk'ubusudizi bw'icyuma kitagira umukungugu gifite 022Cr22Ni5Mo3N.

 

Imiterere ya shimi y'icyuma gisukwa (%):

C

Mn

Si

Cr

Ni

Mo

N

Cu

S

P

≤0.04

0.5 ~ 2.0

≤0.90

21.5 ~ 23.5

8.5 ~ 10.5

2.5 ~ 3.5

0.08 ~ 0.20

≤0.75

≤0.030

≤0.040

 

Imiterere ya tekiniki y'icyuma gisudira:

Ikintu cyo kugerageza

Imbaraga zo gukurura

Mpa

Kurekura

%

Yemejwe

≥690

≥20

 

Ikoreshwa ry'amashanyarazi risabwa:

Umwanya w'inkoni

(mm)

2.5

3.2

4.0

5.0

Umuyoboro wo gusudira

(A)

50 ~70

80 ~ 110

130 ~ 150

160 ~ 200

 

Itangazo:

1. Electrode igomba gutekwa isaha imwe ku bushyuhe bwa 250°C mbere yo gusudira;

2. Ni ngombwa gusukura ingese, ibipimo by'amavuta, amazi, n'imyanda ku bice byo gusudira mbere yo gusudira.

 

 

Wenzhou Tianyu Electronic Co., Ltd. yashinzwe mu 2000. Twakoze akazi ko gukora ibikoresho byaelectrode yo gusudiras, inkoni zo gusudira, naibikoresho byo gusudiraimyaka irenga 20.

Ibicuruzwa byacu by'ingenzi birimo icyuma kitagira umugeseelectrode yo gusudiras, electrode zo gusudira icyuma cya karuboni, electrode zo gusudira zifite alloy nkeya, electrode zo gusudira hejuru, electrode zo gusudira za nikeli na kobalti, insinga zo gusudira zifite icyuma gito n'alloy nkeya, insinga zo gusudira zifite icyuma kidafunze, insinga zikingira gazi, insinga zo gusudira za aluminiyumu, gusudira arc munsi y'amazi. insinga, insinga zo gusudira za nikeli na kobalti, insinga zo gusudira z'umuringa, insinga zo gusudira za TIG na MIG, electrode za tungsten, electrode zo gukata karuboni, n'ibindi bikoresho byo gusudira n'ibindi bikoresho byo gusudira.

 

 


  • Ibanjirije iyi:
  • Ibikurikira: