ER70S2 ni insinga nziza ya MIG na TiG yo gusudira ku byuma byose byoroheje na karuboni, ikora ubusudi bwiza bufite imyenge mike. Ni insinga ya triple deoxidized (Zirconium, Titanium, na Aluminium) ituma iba amahitamo meza yo gusudira hejuru y’ingese n’ubuso bw’icyuma. Nta guhindagurika gukenewe kuri iki gicuruzwa.
IBIKORESHO BYA MBERE:
imiyoboro n'ibikoresho byo gucukura mu mazi, imirimo y'ibyuma by'ubwubatsi
| Aho gusudira: F, V, OH, H | Ubu: DCEP |
| Ingufu zo Gukurura, kpsi: | 70 |
| Imbaraga z'umusaruro, kpsi: | 58 |
| Uburebure muri 2”%: | 22 |
Charpy V-Notch isanzwe: 35 ft.-lb. Kuri -20 deg F
Ubuhanga busanzwe bw'insinga nk'uko bivugwa muri AWS A5.18 (agaciro kamwe ni ntarengwa)
| C | Mn | Si | P | S | Ni | Cr | Mo | V | Cu | Ti | Zr | Al | ||
| 0.07 | 0.90-1.40 | 0.40-0.70 | 0.025 | 0.035 | 0.15 | 0.15 | 0.15 | 0.03 | 0.50 | 0.05-0.15 | 0.02-0.12 | 0.05-0.15 | ||
| Ibipimo bisanzwe byo gusudira | ||||||||||||||
| Ingano | Inzira | Volti | Amps | Gazi yo kurinda | ||||||||||
| in | (mm) | |||||||||||||
| .035 | (0.9) | GMAW | 28-32 | 165-200 | Gutanga spray 98% Argon + 2% Oxygen cyangwa 75% Argon + 25% CO2 | |||||||||
| .045 | (1.2) | GMAW | 30-34 | 180-220 | Gutanga spray 98% Argon + 2% Oxygen cyangwa 75% Argon + 25% CO2 | |||||||||
| 1/16 | (1.6) | GMAW | 30-34 | 230-260 | Gutanga spray 98% Argon + 2% Oxygen cyangwa 75% Argon + 25% CO2 | |||||||||
| .035 | (0.9) | GMAW | 22-25 | 100-140 | Guhindura ikirere gito 100% CO2 cyangwa 75% Argon + 25% CO2 | |||||||||
| .045 | (1.14) | GMAW | 23-26 | 120-150 | Guhindura ikirere gito 100% CO2 cyangwa 75% Argon + 25% CO | |||||||||
| 1/16 | (1.6) | GMAW | 23-26 | 160-200 | Guhindura ikirere gito 100% CO2 cyangwa 75% Argon + 25% CO | |||||||||
| .035 | (0.9) | GTAW | 13-16 | 60-100 | Argon 100% | |||||||||
| .045 | (1.14) | GTAW | 13-16 | 70-120 | Argon 100% | |||||||||
| 1/16 | (1.6) | GTAW | 12-15 | 100-125 | Argon 100% | |||||||||
| 3/32 | (2.4) | GTAW | 15-20 | 125-175 | Argon 100% | |||||||||